Simultaneous measurements of anion self-diffusion and ionic conductivity were performed on pure single crystals, at 440 to 630C, using 36Cl tracers and microtome sectioning (table 177).
M.Bénière, M.Chemla, F.Bénière: Journal of the Physics and Chemistry of Solids, 1979, 40[10], 729-37
Table 177
Ionic Conduction in SrCl2
Temperature (C) | σ (cm2/s) |
441.9 | 1.64 x 10-10 |
473.8 | 8.23 x 10-10 |
504.9 | 1.90 x 10-9 |
532.0 | 5.12 x 10-9 |
557.6 | 1.09 x 10-8 |
585.7 | 2.84 x 10-8 |
598.1 | 1.98 x 10-8 |
609.2 | 2.25 x 10-8 |
629.1 | 7.33 x 10-8 |