Single crystals of perovskite-type compounds in the system, Lix(W1-yNby)O3 (where x
was approximately equal to 0.4 and y ranged from 0 to 0.15), were prepared via the electrolysis of fused salts. The Li-ion conductivity was measured by using a direct-current method and electron-blocking electrodes. A sample with x = 0.4 and y = 0.06 exhibited a conductivity of 1.0 x 10-7S/cm along [100] at room temperature.
Synthesis of Perovskite-Type Single Crystals and their Lithium Ion Conductivity. H.Yamada, M.Hibino, T.Kudo: Journal of the Ceramic Society of Japan, 2001, 109[3], 278-80
Table 136
Ionic Conduction Parameters
for (Li,Zr)YO2 Compositions
Composition | o (S/cm) | E (eV) |
LiYO2 | 0.00268 | 0.68 |
Li0.995Zr0.005Y0.995O2 | 0.00139 | 0.81 |
Li0.95Zr0.05Y0.95O2 | 0.000513 | 0.81 |
Li0.9Zr0.1Y0.9O2 | 0.000912 | 0.87 |
Li1.2Zr0.2Y0.8O2.2 | 0.000797 | 0.88 |
Li1.3Zr0.3Y0.7O2.3 | 0.000861 | 0.92 |